Service · Repointing & restoration

Repointing,done by hand.

Tired mortar lets water in. Scroll and watch the wall behind: old joints are raked out, then lime is pushed back in and struck, one course at a time.

20–25 mmRaked to twice the joint width, no deeper.

LimeSofter than the brick, so the joint wears first.

No grinderChisel and plugging chisel only.

Step 01Look

Read the wall

We scratch the joints with a key. If the mortar crumbles to sand, or the joint is recessed more than a finger-joint deep, it is due. Sound joints are left alone.

Step 02Rake

Rake out

Hand tools, working the perpends first and beds second. A grinder cuts into the brick arris and widens the joint for good, so we do not use one.

Step 03Prepare

Brush & dampen

Dust out, brick wetted so it does not drink the water from fresh lime. Too dry and the new joint fails; too wet and it stains.

Step 04Point

Push, fill, strike

Perpends first, then beds, in layers no thicker than 10 mm. Struck to match the original profile once the mortar is thumb-hard, then brushed back.

Mortar guideTypical, we test each wall

Which lime for which brick

BrickMortarMix by volume
Soft, pre-1900 stocksNHL 2 or lime putty1 : 3
Victorian and Edwardian stocksNHL 3.51 : 2.5
1930s machine-made facingsNHL 3.5 or gauged lime1 : 2 : 8 (cem : lime : sand)
Engineering and hard modernSand and cement, gauged1 : 1 : 6